Electrod Graffit Ffwrnais Diamedr Bach Dwysedd Uchel Ar gyfer Ffwrnais Chwyth Ffwrnais Ladle Mewn Mwyndoddi Dur
Paramedr Technegol
Siart 1: Paramedr Technegol ar gyfer Electrod Graffit Diamedr Bach
Diamedr | Rhan | Gwrthsafiad | Cryfder Hyblyg | Modwlws Ifanc | Dwysedd | CTE | Lludw | |
Modfedd | mm | μΩ·m | MPa | GPa | g/cm3 | ×10-6/℃ | % | |
3 | 75 | Electrod | 7.5-8.5 | ≥9.0 | ≤9.3 | 1.55-1.64 | ≤2.4 | ≤0.3 |
Deth | 5.8-6.5 | ≥16.0 | ≤13.0 | ≥1.74 | ≤2.0 | ≤0.3 | ||
4 | 100 | Electrod | 7.5-8.5 | ≥9.0 | ≤9.3 | 1.55-1.64 | ≤2.4 | ≤0.3 |
Deth | 5.8-6.5 | ≥16.0 | ≤13.0 | ≥1.74 | ≤2.0 | ≤0.3 | ||
6 | 150 | Electrod | 7.5-8.5 | ≥8.5 | ≤9.3 | 1.55-1.63 | ≤2.4 | ≤0.3 |
Deth | 5.8-6.5 | ≥16.0 | ≤13.0 | ≥1.74 | ≤2.0 | ≤0.3 | ||
8 | 200 | Electrod | 7.5-8.5 | ≥8.5 | ≤9.3 | 1.55-1.63 | ≤2.4 | ≤0.3 |
Deth | 5.8-6.5 | ≥16.0 | ≤13.0 | ≥1.74 | ≤2.0 | ≤0.3 | ||
9 | 225 | Electrod | 7.5-8.5 | ≥8.5 | ≤9.3 | 1.55-1.63 | ≤2.4 | ≤0.3 |
Deth | 5.8-6.5 | ≥16.0 | ≤13.0 | ≥1.74 | ≤2.0 | ≤0.3 | ||
10 | 250 | Electrod | 7.5-8.5 | ≥8.5 | ≤9.3 | 1.55-1.63 | ≤2.4 | ≤0.3 |
Deth | 5.8-6.5 | ≥16.0 | ≤13.0 | ≥1.74 | ≤2.0 | ≤0.3 |
Siart 2: Capasiti Cario Presennol Ar gyfer Electrod Graffit Diamedr Bach
Diamedr | Llwyth Cyfredol | Dwysedd Presennol | Diamedr | Llwyth Cyfredol | Dwysedd Presennol | ||
Modfedd | mm | A | Yn2 | Modfedd | mm | A | Yn2 |
3 | 75 | 1000-1400 | 22-31 | 6 | 150 | 3000-4500 | 16-25 |
4 | 100 | 1500-2400 | 19-30 | 8 | 200 | 5000-6900 | 15-21 |
5 | 130 | 2200-3400 | 17-26 | 10 | 250 | 7000-10000 | 14-20 |
Siart 3: Maint a Goddefgarwch electrod graffit ar gyfer electrod graffit diamedr bach
Diamedr Enwol | Diamedr Gwirioneddol(mm) | Hyd Enwol | Goddefgarwch | |||
Modfedd | mm | Max. | Minnau. | mm | Modfedd | mm |
3 | 75 | 77 | 74 | 1000 | 40 | -75~+50 |
4 | 100 | 102 | 99 | 1200 | 48 | -75~+50 |
6 | 150 | 154 | 151 | 1600 | 60 | ±100 |
8 | 200 | 204 | 201 | 1600 | 60 | ±100 |
9 | 225 | 230 | 226 | 1600/1800 | 60/72 | ±100 |
10 | 250 | 256 | 252 | 1600/1800 | 60/72 | ±100 |
Prif Gais
- Mwyndoddi calsiwm carbid
- Cynhyrchu carborundwm
- Coethi corundum
- Metelau prin yn toddi
- Planhigyn Ferrosilicon anhydrin
Rhoi cyfarwyddiadau a defnyddio ar gyfer electrodau graffit
1.Defnyddiwch yr offer codi arbennig i fywyd yr electrod graffit osgoi difrodi yn ystod cludiant. (gweler llun 1)
2. Rhaid cadw electrod graffit i ffwrdd rhag cael ei wlychu neu ei wlychu gan law, eira, ei gadw'n sych. (gweler llun 2)
3. Gwiriwch yn ofalus cyn ei ddefnyddio, sicrhewch fod y soced a'r deth yn addas i'w defnyddio, gan gynnwys archwilio traw, plwg. (gweler llun 3)
4.Glanhewch edafedd y deth a'r socedi ag aer cywasgedig. (gweler llun 4)
5. Cyn ei ddefnyddio, rhaid i'r electrod graffit gael ei sychu yn y ffwrnais, dylai'r tymheredd sychu fod yn llai na 150 ℃, dylai'r amser sychu fod yn fwy na 30 awr. (gweler pic5)
6. Rhaid cysylltu electrod graffit yn dynn ac yn syth gyda trorym tynhau addas. (gweler pic6)
7. Er mwyn osgoi'r toriad electrod graffit, rhowch y rhan fawr yn y safle isaf a rhan fach yn y safle uchaf.